Carbon Plus Case Study 3: High Power Durability Test of Carbon Plus vs OEM Friction Material
Overview
At Industrial Brake & Friction Supply, we are committed to supplying high-performance, rigorously tested friction materials to the heavy equipment industry. This case study highlights the results of an SAE No.2 High Power Durability Test comparing two materials: Carbon Plus (our advanced Carbon Composite friction material) and an OEM Graphite Friction Material (a standard haul truck transmission benchmark material).
Test Overview
The test was designed to simulate extreme working conditions using UTTO oil and measured several key performance indicators over 10,000 cycles.
Test Conditions:
- Dynamic RPM: 3600
- Inertia: 0.490 kgf.m.sec²
- Absorbed Power (Break-in): 130.1 W/cm²
- Absorbed Energy (Durability): 216.5 W/cm²
- Oil Flow Rate: 2.57 L/min @ 115°C
- Plate Dimensions: 146.15 mm OD / 120.55 mm ID
- 6 EA Disc surfaces
1. Break-In Performance
During the break-in stage, Carbon Plus maintained a stable and predictable coefficient of friction (μ), showing minimal fluctuation. OEM Friction Material began to show a slight upward trend in μ, indicating earlier wear or surface instability.
2. Dynamic Friction (Durability Stage)
At 216.5 W/cm²:
Carbon Plus maintained consistent friction levels with a gradual increase in performance over time.
OEM Friction Material experienced a noticeable decline and ultimately suffered damage before completing the full cycle.
3. Static Friction (Durability Stage)
Carbon Plus again outperformed OEM Friction Material, showing better stability and grip throughout the test cycles. OEM Friction Material’s performance degraded steadily.
4. μ-V Characteristics
Carbon Plus demonstrated excellent consistency in torque control and responsiveness across all test stages. In contrast, OEM Friction Material‘s μ-V performance was less predictable and started to degrade under sustained load.
5. Wear Comparison
One of the most important test metrics, material wear, clearly highlighted the durability of Carbon Plus:
Carbon Plus showed minimal wear over 10,000 cycles, reducing gradually from 0.106 mm to 0.030 mm.
OEM Friction Material exhibited more aggressive wear, with the test halted at 8,000 cycles due to part failure.
6. Visual Condition After Test
Carbon Plus components remained intact and visibly less worn even after 10,000 cycles.
OEM Friction Material components showed clear damage and surface breakdown by 8,000 cycles.
7. Dynamic Torque Trace
Carbon Plus maintained stable torque delivery at all stages, from break-in to 10,000 cycles. OEM Friction Material, however, showed increasingly erratic torque characteristics before complete failure.
Conclusion
The results of this SAE High Power Durability Test demonstrate a clear and measurable advantage of Carbon Plus over the OEM graphite-based friction material. Across every critical performance metric: dynamic and static friction, wear resistance, torque stability and surface integrity, – Carbon Plus consistently delivered superior results under demanding, high-power conditions.
Most notably, Carbon Plus maintained predictable, high-friction coefficients and minimal wear throughout the entire 10,000-cycle test, while the OEM material experienced progressive performance degradation and ultimately failed before reaching the test limit. The visual integrity of Carbon Plus discs post-test further underscores its robustness and suitability for heavy-duty transmission applications where reliability and service life are paramount.
For operators seeking to reduce downtime, extend maintenance intervals and improve long-term cost efficiency Carbon Plus represents a premium aftermarket solution that exceeds OEM performance. Backed by thorough testing and proven in real-world environments, it is an ideal choice for high-inertia, high-heat and high-load applications across mining, construction, and heavy transport.